Cutting and Drilling Hardox: Preheating, HAZ and Method Selection

In short: Hardox® wear steel can be cut by oxy-fuel, plasma, laser and abrasive waterjet. Hardox gets its hardness from quenching and is tempered at a relatively low temperature. In thermal cutting, two risks must therefore be watched: softening of the cut edge or of a small part and delayed hydrogen cracking at the cut edge. SSAB's measures are preheating according to thickness and grade, a cutting sequence that spreads the heat over the plate, a maximum temperature limit and slow cooling after cutting. For example, Hardox 450 up to 39.9 mm is cut without preheating, while Hardox 500 over 60 mm requires at least 175 °C.

The values in this guide are taken from SSAB's cutting and machining pages. In the interactive model below you can choose the grade, thickness and cutting method and follow the process step by step: preheating, cutting, heat-affected zone, part temperature check and slow cooling.

3D model: thermal cutting of Hardox step by step — from preparation to slow cooling

3B model hazırlanıyor…

  1. Levha oda sıcaklığında olmalıdır; dışarıda ya da soğuk ortamda beklediyse kesimden önce oda sıcaklığına getirilir. Oksijenle kesimde yüzey durumunun etkisi sınırlıdır; boyalı ya da paslı yüzeyde kesme hızı biraz düşürülebilir.

  2. Levha en az 100 °C'ye, en fazla 225 °C'ye ısıtılır. Sıcaklık tüm kesitte sağlanmalıdır; ısıtılan yüzün karşı tarafından ölçülür. En düzgün ısınmayı fırın sağlar; elektrikli battaniyeler yavaş ısıttığı için SSAB gece boyu ısıtmayı önerir.

  3. Alev levhayı tutuşma sıcaklığına (≈ 900 °C) ısıtır, kesme oksijeni eriyen metali üfler. Kesme hızı ile kesme oksijeni basıncı birbirine uygun olmalıdır: yüksek hız yüksek basınç ister. İçe bakan keskin köşelerden kaçınılır; yumuşak geçişler gerilimi dağıtır. Kesim yarıda kalacaksa (ör. gece) kesik temiz bir kesimle bitirilir.

  4. Kesik kenarında ısıdan etkilenen bölge (ITAB) oluşur; oksijen için yaklaşık 4–10 mm. Kenara en yakın kısım (SSAB'nin örneğinde ≈ 1–2 mm) 900 °C'nin üstüne çıkar, hızla soğuyup yeniden sertleşir (bölge 1). Arkasındaki bölge 900 °C'nin altında kalır ve menevişlenip yumuşar (bölge 2).

  5. Parçanın sıcaklığı kesimden hemen sonra ölçülür; en fazla 225 °C olmalıdır, üstüne çıkarsa sertlik düşer. Isıyı dağıtmak için sıradaki parça levhanın uzak köşesinden kesilir ya da levhanın soğuması beklenir. Oksijenle 30 mm ve üstünde iki kesim arası 200 mm'den azsa parçanın tamamı yumuşayabilir; bu parçanın dar kenarı 380 mm. Su altında kesim ya da su püskürtme parçanın tamamen yumuşamasını önler, ama kenarda 5–10 mm'lik yumuşak bölge yine oluşur.

  6. Ön ısıtma yapılsın ya da yapılmasın yavaş soğutma kesik kenarında çatlak riskini azaltır: sıcak parçalar üst üste istiflenip yalıtım örtüsüyle örtülür ve oda sıcaklığına yavaşça iner. Son ısıtma gerekirse fırında en az 200 dk (5 dk/mm), en fazla 225 °C; torçla yapılırsa kenar 700 °C'yi geçmemeli, tercihen 300–500 °C'de (çok koyu kırmızı) tutulmalıdır.

Kendi kesiminizi seçin

Kesim yöntemi
Ön ısıtma (SSAB tablosu)
en az 100 °C
En yüksek sıcaklık
225 °Cön/son ısıtma, parça
Isıdan etkilenen bölge
≈ 4–10 mm
Fırında son ısıtma
en az 200 dk5 dk/mm

Oksijenle ≥ 30 mm: iki kesim arası 200 mm’den az olan parçalar tamamen yumuşayabilir. Kaynak: SSAB ön ısıtma · SSAB ITAB

The model animates the sequence recommended by SSAB in six steps: preparing the plate at room temperature, preheating if required and measuring on the opposite surface, cutting, the heat-affected zone at the cut edge, part temperature and dimension check, and slow cooling by stacking and covering. When you change the grade, thickness and cutting method, the values in the steps update according to the SSAB table. Şematik model: 1400 × 900 mm levhadan 600 × 380 mm (köşe R80) parça. ITAB bantları 5 kat büyütülmüştür; termal renkler ve ara sıcaklık okumaları örnektir. Hedef değerler (ön ısıtma, en yüksek sıcaklık, ITAB aralığı, son ısıtma süresi) SSAB'den alınmıştır.

Which cutting method?

According to SSAB there is no single best method; the most common compromise is probably oxy-fuel cutting. Plate thickness, tolerance, edge quality, plate hardness, heat effect, cost and available equipment are decisive in the choice. Heat input varies from method to method: oxy-fuel cutting gives the most heat, then plasma, and laser the least; waterjet is a cold method.

Method

SSAB's guideline thickness range

Heat-affected zone (HAZ)

Preheating

Oxy-fuel cutting

over 10 mm (above 50 mm the only option together with waterjet)

4–10 mm

Applied according to the table

Plasma, oxygen gas

up to 50 mm

2–5 mm

Applied according to the table

Plasma, nitrogen gas

up to 50 mm

2–5 mm

Not recommended (edge quality)

Laser

up to 30 mm

0.2–2 mm

Not recommended (edge quality)

Abrasive waterjet

over 3 mm

0 mm

Not required

SSAB's list by thickness: below 2 mm laser; below 3 mm plasma or laser; below 10 mm waterjet, plasma or laser; above 10 mm laser, plasma, oxy-fuel or waterjet; above 30 mm plasma, oxy-fuel or waterjet; above 50 mm oxy-fuel or waterjet.

Surface condition: In oxy-fuel and plasma cutting the effect of the surface is limited; on painted or rusty surfaces the oxy-fuel cutting speed may be reduced slightly. In laser cutting, however, surface cleanliness is the most important factor; the area around the cutting line must be completely free of paint, rust and dirt. In plasma cutting the earth clamp is connected directly to the plate being cut; for SSAB steels the same consumables and settings as for mild steel can generally be used, though fine adjustment of speed, current and gas flow may be needed.

Preheating before thermal cutting

Preheating allows more hydrogen around the cut to diffuse out and reduces the cooling rate of the cut edge, lowering the resulting tensile stresses. According to SSAB, preheating is especially beneficial in oxy-fuel cutting and plasma with oxygen gas. It is not recommended for laser and plasma with nitrogen gas, because it impairs edge quality.

Grade

Plate thickness (mm)

Minimum preheat

Maximum temperature

Hardox HiTuf

up to 89.9

Not required

300 °C

Hardox HiTuf

90–150

100 °C

300 °C

Hardox HiAce

up to 39.9

Not required

225 °C

Hardox HiAce

40–49,9

100 °C

225 °C

Hardox HiAce

50–69,9

150 °C

225 °C

Hardox HiAce

70–100

175 °C

225 °C

Hardox 400

up to 44.9

Not required

225 °C

Hardox 400

45–59,9

100 °C

225 °C

Hardox 400

60–80

150 °C

225 °C

Hardox 400

81,1–150

175 °C

225 °C

Hardox 450

up to 39.9

Not required

225 °C

Hardox 450

40–49,9

100 °C

225 °C

Hardox 450

50–69,9

150 °C

225 °C

Hardox 450

70–150

175 °C

225 °C

Hardox 500 Tuf

4–25,4

Not required

225 °C

Hardox 500

up to 24.9

Not required

225 °C

Hardox 500

25–49,9

100 °C

225 °C

Hardox 500

50–59,9

150 °C

225 °C

Hardox 500

60–150

175 °C

225 °C

Hardox 550

up to 19.9

Not required

200 °C

Hardox 550

20–51

150 °C

200 °C

Hardox 550

51,1–150

175 °C

200 °C

Hardox 600

up to 11.9

Not required

180 °C

Hardox 600

12–65

170 °C

180 °C

Hardox 400, 450, 500, 500 Tuf, 600 and HiAce sheet (2–10 mm) and Hardox 450 cold-rolled sheet (0.8–2.1 mm) are cut without preheating. The maximum temperature column is the limit that must not be exceeded during preheating and post-heating; above it, the hardness of the steel drops.

This preheating table is for thermal cutting. Preheating values before welding are different; see Hardox welding.

How is preheating done?

  • Room temperature requirement: Even if no preheating is required, the plate must be at room temperature when cut. A plate that has cooled down outdoors or in an unheated area is brought to room temperature before cutting.
  • Furnace: The best method, because it gives an even temperature over the whole plate.
  • Heating torch: Can be used, but the torch must be kept moving; otherwise the plate may exceed the maximum temperature.
  • Electric heating blanket: Temperature control is precise, but heating is slow. SSAB recommends heating the plate overnight to reach 150–200 °C and starting cutting in the morning.
  • Measurement: Preheating must be achieved through the whole section. The temperature is measured on the opposite side from the heated face.
  • Soaking time: After the surface reaches the target temperature, wait a while for the core to heat up too. SSAB's example: if a 100 mm plate is heated from both sides to 175 °C, this temperature is held for 11 minutes after the surface reaches 175 °C.

Heat-affected zone (HAZ) and softening

Thermal cutting leaves a HAZ at the cut edge regardless of steel grade. In quenched steels this zone is divided into two:

  • Zone 1 (re-hardened): The outermost part, about 1–2 mm in from the cut edge. During cutting it rises above 900 °C and, because the heat spreads rapidly into the plate as the torch advances, it hardens as if re-quenched. The hardness and strength of this zone are higher than those of the base metal.
  • Zone 2 (tempered): Lies between Zone 1 and the unaffected base metal, is heated below 900 °C and tempered. Its hardness varies with the steel grade and cutting efficiency.

The HAZ width depends on grade, thickness and heat input. Typical values given by SSAB: 4–10 mm for oxy-fuel cutting, 2–5 mm for plasma, 0.2–2 mm for laser, 0 mm for waterjet.

Softening of the whole part in small parts

The smaller the cut part, the more the heat from preheating and cutting accumulates in it; the whole part may soften. SSAB's rule of thumb: when oxy-fuel cutting plate of 30 mm and above, if the distance between two cuts is less than 200 mm there is a risk of hardness loss in the whole part. Below 30 mm, smaller parts can be cut without hardness loss. An easy way to tell whether a part is too small is to measure its temperature immediately after cutting.

Preventing softening

  • Cold cutting: The best way to eliminate the risk completely is abrasive waterjet. If thermal cutting is required, laser or plasma is preferred to oxy-fuel cutting.
  • Water cooling: In oxy-fuel cutting, cutting the plate under water or spraying water during and after cutting limits the soft zone and prevents the whole part from softening. Even so, a soft zone of about 5–10 mm forms at the cut edge, because the flame and cutting oxygen push the water away from the cutting front.
  • Cutting sequence (nesting): If all parts are cut one after another from one end of the plate, the first part keeps its hardness, but subsequent parts may soften because they are cut from an increasingly hot plate. After cutting a part from one corner, the next part should be cut from the opposite corner, or the plate should be allowed to cool.

Advantages of underwater cutting: prevents the whole part from softening, reduces distortion, parts cool immediately, no fumes or dust, less noise. Because preheating cannot be applied under water, the remaining measures against hydrogen cracking are post-heating and a low cutting speed.

Preventing cracks at the cut edge

Hydrogen cracking is a type of crack that can appear with a delay of several days after thermal cutting. Cutting brings hydrogen to the edge, the temperature accelerates hydrogen diffusion, and tensile stress remains around the cut. Especially in hard steel, the conditions for cracking are thus created. The additional measures recommended by SSAB are preheating, post-heating and slow cooling.

  • Slow cooling: Whether or not preheating is done, slow cooling reduces the risk of cracking at the cut edge. The hot parts coming off the cutting table are stacked on top of each other and covered with an insulating blanket to cool slowly to room temperature.
  • Post-heating in a furnace: The time is roughly at least 5 minutes per mm of thickness (50 minutes for a 10 mm plate). The minimum and maximum temperatures are the same as in the preheating table. An inexpensive set-up can be built with a heating box, electric heaters and insulating blankets such as rock wool.
  • Post-heating with a torch: The temperature of the cut edge must not exceed 700 °C and should preferably be kept at 300–500 °C. Under the torch the edge should glow a very dark red; bright cherry red or dark orange indicates the temperature is too high. The temperature can also be monitored with an infrared thermometer. A large, low-intensity flame lets the heat penetrate deeply without overheating.
  • Corners: Sharp inward-facing corners concentrate stress and can be crack initiation points. Use smooth, continuous transitions; if a sharp corner is unavoidable, move the torch around outward-facing corners in a small loop.
  • Interruptions: If cutting is to be interrupted (e.g. overnight), the cut is completed with a clean cut so that half cuts do not create stress concentrations.

Reducing distortion

Because high-strength steel is more resistant to yielding, it can distort more than mild steel in thermal cutting; thick plate distorts less because of its rigidity. SSAB's recommendations:

  • If no preheating is required, cut under water. If preheating or post-heating is required, cutting under water followed by post-heating reduces distortion more than preheating.
  • Switch to a method with less heat: oxy-fuel → plasma → laser.
  • Use a nesting layout that cuts parts from different areas of the plate.
  • For long, narrow parts, cut both edges simultaneously with two torches where possible.
  • Heat-free methods (waterjet, saw) eliminate distortion completely.

Drilling Hardox

According to SSAB, Hardox is a long-chipping material; in drilling, machine rigidity, tool clamping and cooling are decisive.

  • Drill selection: If machine conditions are good, always choose a cemented carbide drill: solid carbide drills for small diameters and tight tolerances, exchangeable-tip drills for medium diameters, and indexable insert drills for low cost per hole. With exchangeable-tip and indexable drills, the body should be kept as short as possible.
  • Non-rigid machine (pillar/radial drill): Only in this case use HSS-Co (8% Co) drills; choose those with a small helix angle and a thick, torque-resistant core. HSS-Co drills are only suitable up to 500 Brinell and can drill a few holes before regrinding.
  • Tool clamping: A Morse taper connection is not rigid and is suitable for HSS drills. Hydraulic or shrink-fit chucks reduce runout. Tool runout must not exceed 0.02 mm.
  • Cooling: The most common cutting fluid is emulsion; when drilling Hardox the mixing ratio should be 8–12%. Internal cooling is always preferred to prevent chip jamming; deep holes need high emulsion pressure.
  • Chip breaking: If the chips do not break, increase the feed or reduce the cutting speed; the chip becomes thicker and breaks more easily. Peck drilling also breaks the chips, but wears the drill faster in hardened steel such as Hardox.
  • Workpiece: Clamping must suit the shape of the part; a poorly clamped part vibrates, spoils the hole surface and shortens tool life.

Cutting speed and feed values should be chosen according to the drill manufacturer and SSAB's Machining recommendations for Hardox brochure.

Frequently Asked Questions

How is Hardox plate cut?

Hardox can be cut by oxy-fuel, plasma, laser and abrasive waterjet. According to SSAB's guideline list, laser is suitable up to 30 mm and plasma up to 50 mm; above 50 mm oxy-fuel or waterjet is used. Laser gives the least heat; waterjet is a cold method and leaves no heat-affected zone.

Is preheating required before cutting Hardox?

It depends on grade and thickness. According to SSAB, Hardox 400 is cut without preheating up to 44.9 mm, Hardox 450 up to 39.9 mm, Hardox 500 up to 24.9 mm, Hardox 550 up to 19.9 mm and Hardox 600 up to 11.9 mm; Hardox 500 Tuf needs no preheating over its whole range (4–25.4 mm). Thicker plate requires 100–175 °C. Preheating is applied in oxy-fuel cutting and plasma with oxygen gas; it is not recommended for laser and plasma with nitrogen gas.

What preheat temperature is used when cutting Hardox 500?

According to SSAB, Hardox 500 plate needs no preheating up to 24.9 mm; 100 °C is applied at 25–49.9 mm, 150 °C at 50–59.9 mm and 175 °C at 60–150 mm. The maximum temperature is 225 °C.

Does Hardox lose its hardness in laser cutting?

Laser is the thermal method that gives the least heat; according to SSAB the heat-affected zone is 0.2–2 mm (2–5 mm for plasma, 4–10 mm for oxy-fuel cutting). The part of this zone closest to the edge re-hardens, and the part behind it is tempered and softens. If heat accumulates in small parts, the whole part may soften; the cutting sequence should therefore be planned to spread the heat over the plate.

How wide is the heat-affected zone (HAZ)?

Typical values given by SSAB: 4–10 mm for oxy-fuel cutting, 2–5 mm for plasma, 0.2–2 mm for laser, 0 mm for waterjet. The width depends on grade, thickness and heat input.

Why do small Hardox parts soften?

The heat from preheating and cutting accumulates in a small part. According to SSAB, when oxy-fuel cutting plate of 30 mm and above, if the distance between two cuts is less than 200 mm there is a risk of hardness loss in the whole part. The solution is waterjet, laser or plasma, underwater cutting, or a cutting sequence that spreads the heat over the plate.

Why do cracks form at the Hardox cut edge?

Thermal cutting brings hydrogen to the edge and leaves tensile stress; in hard steel this can lead to hydrogen cracking with a delay of several days. SSAB's measures are preheating, post-heating (in a furnace at least 5 min/mm) and slow cooling: hot parts are stacked and covered with an insulating blanket.

What drill is used to drill Hardox?

According to SSAB, if machine conditions are good, cemented carbide drills should be used: solid, exchangeable-tip or indexable insert. On a non-rigid machine HSS-Co (8% Co) drills can be used, but these drills are only suitable up to 500 Brinell. The emulsion ratio should be 8–12%, internal cooling should be preferred and tool runout must not exceed 0.02 mm.

Hardox cutting at Sacdan Adam

For cutting, bending and welded assembly of Hardox plates from stock, see the Hardox laser cutting page or fill in the quotation form.

Related pages

Hardox welding · Hardox bending · Choosing Hardox by wear type · Hardox 450 · Hardox 500

Sources

The technical values on this page were read directly from the following SSAB pages (accessed: 5 November 2026). SSAB updates its recommendations from time to time; use the latest version for production.

Hardox® is a trademark of the SSAB group. This page has been prepared for general technical information; Sacdan Adam cannot be held liable for any damage arising from decisions taken on the basis of the information given here.